spt-blog-banner-14

Sacrificial Layer Etching in MEMS with Aluminum Interconnects

Sacrificial Layer Etching in MEMS with Aluminum Interconnects

In MEMS sacrificial layer etching, extra precautions are required when handling structures featuring aluminum interconnects. In CMOS-integrated MEMS, Al is often exposed on the wafer surface, creating a high risk of corrosion by the chemicals or gases used to remove sacrificial layers. This article outlines essential strategies for removing sacrificial layers without damaging Al interconnects, covering etching methodologies, reaction by-product moisture, sacrificial layer film quality, protective layer selection, and reliability evaluation.

Why Aluminum Interconnects Are Vulnerable During MEMS Sacrificial Layer Etching

What Is Sacrificial Layer Etching?

In surface-micromachined MEMS, a sacrificial layer—typically silicon dioxide (SiO₂)—is temporarily deposited underneath or around structural layers and selectively removed in the final fabrication phase. This process releases suspended movable structures such as cantilevers and membranes into free space. Sacrificial layer etching is widely recognized as a core process in MEMS surface micromachining(Source:International Core Journal of Engineering「MEMS Sacrificial Layer Release Technology」).

Exposed Al Interconnects in CMOS-MEMS

In recent years, the integration of MEMS and CMOS circuits onto a single chip ("CMOS-MEMS") has gained significant traction. Aluminum serves as the standard interconnect material in CMOS fabrication. Consequently, sacrificial layer etching must frequently be performed with Al exposed on the device surfaceす(Source:Idonus「Etch stop materials for release by vapor HF etching」).

This requires exceptionally high etch selectivity: removing only the sacrificial layer while leaving the Al unaffected. Prioritizing countermeasures depends on structural variables such as the degree of exposed Al pads/lines and direct contact with dissimilar metals.

In Automotive Applications, Even Trace Damage Undermines Reliability

The global MEMS market is projected to reach $17.1 billion in 2025 and grow to $24.0 billion by 2031. In the automotive sector, the adoption of inertial measurement units (IMUs) and pressure sensors continues to rise alongside vehicle electrification and advanced driver-assistance systems (ADAS) (Source:Yole Group「Status of the MEMS Industry 2026」).

Automotive-grade devices must comply with rigorous reliability standards, such as AEC-Q100(Source:OKI Engineering, "AEC-Q100 Testing"). Even minor corrosion initiated during sacrificial layer etching can manifest as a fatal defect during subsequent reliability qualification.

Two Critical Requirements

This article focuses on simultaneously fulfilling two essential criteria:

  • Zero damage to Al interconnects (avoiding corrosion, pitting, or film thinning).
  • Reliable release of mechanical microstructures from the substrate.

Dry vs. Wet Etching: Can You Protect Aluminum Interconnects?

While "dry etching" generally refers to plasma-based processes, in sacrificial layer etching it often denotes non-liquid vapor-phase etching (such as anhydrous HF vapor). This article uses "dry" in this vapor-phase sense.

Wet Etching: Aqueous HF Directly Dissolves Aluminum

Aqueous hydrofluoric acid (HF) has traditionally been used to remove SiO₂ sacrificial layers(Source:Google Patents「US20090308843A1」). However, Al is vulnerable to aqueous HF solutions, etching isotropically at roughly 11 nm/min in 5:1 dilute HF(Source:memsstar「HF Acid Etch vs HF Vapor Etch」"https://memsstar.com/hf-acid-etch-vs-hf-vapour-etch/").

Structures or processes requiring longer etch times prolong chemical exposure, elevating the risk of line thinning and open-circuit failures alongside process duration.

Often-Overlooked Galvanic Corrosion

In wet processes, galvanic corrosion (bimetallic corrosion) presents an even greater hazard. When Al makes electrical contact with noble or dissimilar metals (such as Au, Cr, or Ti) in an electrolyte, potential differences establish localized galvanic cells. In this state, Al acts as the anode (the dissolving electrode) due to its lower electrochemical potential, drastically accelerating dissolution(Source:Nihon Barrel Kogyo,"Galvanic Corrosion ").

Studies using multilayer metal stacks for MEMS demonstrate that Al films in contact with dissimilar metals etch significantly faster than single-layer Al films. Acceleration rates depend on metal combinations, etchant chemistry, and anode-to-cathode surface area ratios(Source:A. Ravi Sankar, S. Das「Experimental analysis of galvanic corrosion of a thin metal film in a multilayer stack for MEMS application」Materials Science in Semiconductor Processing).

In practice, evaluating etch rates on blanket Al films alone is insufficient to predict damage on actual devices. When designing electrodes or interconnects with heterogeneous metals, accelerated corrosion must be factored in, even if single-film test specimens show no adverse effects.

Wet Etching with Specialized Drying: Alternatives and Limitations

Supercritical CO₂ (sCO₂) drying is often employed to mitigate stiction while retaining wet chemistry. Above its critical point (31.1℃, 7.38 MPa), CO₂ exhibits no surface tension between gas and liquid phases, eliminating capillary forces during release. However, integrating this into high-volume manufacturing lines requires costly, specialized high-pressure chambers. Furthermore, solvent exchange from alcohol to liquid CO₂ is time-consuming, introducing significant throughput and operational cost bottlenecks (Source:PatSnap「Pattern Collapse Mitigation: Supercritical CO2 Drying Techniques」)。

Moreover, using advanced drying does not change the fact that aqueous HF directly contacts Al during etching. When selecting a method, drying-induced stiction and chemical corrosion must be treated as distinct challenges.

Dry Etching (Anhydrous HF Vapor): Protective Passivation on Aluminum

In vapor-phase etching using anhydrous HF vapor, an ultra-thin aluminum fluoride (AlF₃) passivation film forms on the Al surface, halting further reaction and virtually eliminating Al loss. Additionally, operating entirely in the vapor phase inherently eliminates stiction caused by capillary forces(Source:Idonus「Etch stop materials for release by vapor HF etching」)。

Comparison: Etching Methods for Structures with Al Interconnects

Wet Etching (Aqueous HF) Dry Etching (Anhydrous Vapor HF)
Impact on Al Isotropically etched (~11 nm/min in 5:1 DHF) Virtually unetched due to protective AlF₃​ passivation
Dissimilar Metal Contact High risk of accelerated galvanic corrosion No liquid medium; risk minimized (condensation must be managed)
Drying Process High stiction risk during rinse/dry (sCO₂​ requires expensive, slow tooling) Completely dry; no drying step required
Key Process Controls Chemical exposure time, metal stack composition Temperature and pressure regulation to prevent moisture condensation

For structures with exposed Al—especially those contacting dissimilar metals—dry etching (anhydrous Vapor HF) is the optimal choice. However, dry etching is not unconditionally immune to issues. Below are four key technical considerations when running vapor-phase processes.

Consideration 1: Reaction-Generated Moisture Can Corrode Aluminum

The reaction between HF vapor and SiO is expressed as "SiO₂+4HF→SiF₄(gas)+2H₂O". Water is formed as an unavoidable reaction by-product(Source:Google Patents「US20090308843A1」). If chamber temperature and pressure are improperly controlled, this water condenses on the wafer surface, creating localized aqueous HF droplets. This can trigger galvanic corrosion of Al, even inside a "dry" chamber(Source:Academia.edu「Dry release for surface micromachining with HF vapor-phase etching」).

To prevent this, process gases are dosed with alcohol vapors (such as methanol or ethanol) to regulate condensation while driving the reaction(Source:ResearchGate「Highly selective isotropic gas-phase etching of SiO2 using HF and methanol at temperatures -30 °C and lower」).

While moisture condensation is a known cause of stiction, in structures containing Al it manifests as chemical corrosion. Even when a release appears dry and successful under optical inspection, the physical state of the Al surface must be rigorously verified.

Consideration 2: Verify the Sacrificial SiO₂ Deposition Method

Different deposition techniques yield SiO₂ films with divergent behaviors under HF vapor exposure. Research by the VTT Technical Research Centre of Finland shows that thermal oxide and LPCVD (low-pressure CVD) oxides etch stably without leaving residue on Al surfaces. Conversely, PECVD (plasma-enhanced CVD) oxides (e.g., TEOS-based oxides) feature high hydrogen content and lower film density, which frequently generate corrosive residues on Al surfaces post-etch(Source:VTT「Studies on aluminium corrosion during and after HF vapour treatment」).

If residues persist despite tuning etching parameters, the root cause often lies in film density and stoichiometry rather than chamber recipes. Clearly defining deposition methods alongside etch parameters during initial development accelerates root-cause diagnosis.

Consideration 3: Select Protective Layers Based on SiN and Al₂O₃ Properties

When adding etch-stop or passivation layers to shield CMOS circuits and Al lines, verify their chemical resistance to HF vapor:

  • Silicon Nitride  (SiN): Although widely used, SiN reacts gradually with HF vapor to yield solid ammonium fluorosilicate ((NH₄)₂SiF₆) by-products(Source:Google Patents「EP1700822B1」).

  • Aluminum Oxide (Al₂O₃): Ultra-thin Al₂O₃ films grown by ALD (Atomic Layer Deposition) are chemically inert to HF vapor, serving as robust passivation barriers for underlying CMOS circuits(Source:ResearchGate「Etch stop materials for release by vapor HF etching」).

When using silicon nitride, evaluate not only its etch resistance but also whether solid reaction by-products deposit on the device.

Consideration 4: Design Etch Criteria Backward from Reliability Testing

Automotive reliability qualifications subject devices to rigorous environmental stress screening, including temperature cycling and high-humidity/high-temperature storage. Representative AEC-Q100 test conditions include(Source:Renesas Electronics, "R7F7010233AFD-C Reliability Report for AEC-Q100").

Representative Parameters Potential Risks Originating from Sacrificial Etch
Temperature Cycling (TC) -55℃〜150℃, 1000 cycles Micro-corrosion on Al serves as stress-concentration points, leading to thermal cracks and line breakage.
High Humidity / High Temp 85℃/85%RH(THB)、110℃/85%RH(UHST) Residual fluorine compounds absorb moisture, inducing electromigration and leakage currents.
Shock & Vibration Mechanical screening for cavity packages Residual mechanical stresses in released structures can cause structural rupture.

Note: The risks listed above represent failure mechanisms derived from historical defect physics. Specific causal relationships must be verified on actual device structures.

Even if post-release optical inspection shows clean devices, latent micro-corrosion and chemical residues can cause premature failures under stress. Factoring qualification tests into sacrificial etch optimization mitigates costly redesign loops downstream.

Troubleshooting Guide: Symptoms & First-Check Points

Use this guide as an initial checklist when issues occur in production or development:

First Check Point Related Consideration
Al pads/lines corrode despite using a dry process Check chamber temperature and pressure to ensure reaction by-product moisture is not condensing on the wafer. Point 1
Corrosion is localized exclusively at dissimilar metal junctions Galvanic corrosion. Verify whether condensed moisture or liquid bridged the Al and adjacent noble metals. Wet vs. Dry , Point 1
Post-etch residues remain on the Al surface Confirm whether the sacrificial layer is a PECVD oxide (e.g., TEOS) with low film density. Point 2
Solid crystalline by-products appear on passivation layers Confirm whether silicon nitride (SiNSiN) was used, which reacts with HF vapor to form solid residues. Point 3
Devices pass post-release visual inspection but fail reliability tests Inspect for sub-micron Al corrosion pits or residual fluorinated compounds using TEM/EDX or XPS. Point 4

Frequently Asked Questions (FAQ)

 A. While anhydrous HF vapor naturally forms a protective AlF₃ passivation layer on aluminum, secondary corrosion can still occur if reaction-generated moisture (H₂O) condenses on the wafer. Maintaining precise thermal and pressure controls with appropriate alcohol vapor additives is necessary to keep the environment strictly gas-phase. 

 A. It can be used, but PECVD oxides (including TEOS) contain higher hydrogen content and lower density than thermal or LPCVD oxides, making them prone to leaving corrosive residues on Al surfaces. If PECVD oxide must be used, etch recipes must be finely tuned, or post-deposition annealing should be considered. 

 A. Al₂​O₃​ deposited via ALD is strongly recommended. While SiNSiN is widely accessible, it reacts with HF vapor over prolonged exposures to produce solid ammonium fluorosilicate residues. ALD Al₂O₃​ remains inert and residue-free. 

 A. No. While sCO₂drying prevents capillary-induced stiction, it does not prevent chemical attack or galvanic corrosion while the device is immersed in the aqueous HF bath prior to drying. For structures with exposed Al, vapor HF etching remains the superior technical solution. 

"Vetelgeuse": Advanced Sacrificial Layer Etcher for MEMS with Al Interconnects

The Vetelgeuse sacrificial layer etching system from Sumitomo Precision Products employs a fully dry process using anhydrous HF vapor to isotropically remove SiO₂ sacrificial layers. Engineered specifically for devices containing aluminum structures, it selectively strips oxides without causing galvanic corrosion or chemical damage. Operating completely liquid-free, it eliminates stiction while delivering large undercut cavities—ranging from micrometers to millimeters—in a single vapor-phase process.

Built for high-volume manufacturing, Vetelgeuse utilizes the vacuum-transfer VPX Platform, supporting up to three integrated process chambers. By transferring wafers continuously under high vacuum, it prevents ambient moisture adsorption, maximizing process repeatability. The system generates zero liquid chemical waste. Its architecture addresses the critical moisture management highlighted in Consideration 1, not only via recipe optimization but through atmospheric vacuum isolation.

Summary

  • When etching sacrificial layers in MEMS with exposed Al interconnects, processes must deliver damage-free selectivity alongside reliable mechanical release.

  • Aqueous HF wet etching attacks aluminum directly, while dissimilar metal contacts drive accelerated galvanic corrosion. Supercritical CO₂ drying eliminates stiction, but does not prevent chemical attack during immersion.

  • Anhydrous HF vapor dry etching provides superior compatibility with Al, though reaction by-product moisture condensation must be tightly suppressed.

  • Film properties dictated by deposition methods (thermal/LPCVD vs. PECVD) and protective layer materials (SiN vs. Al₂O₃) govern post-etch residue and corrosion outcomes.

  • For automotive applications, tuning etch parameters with post-release reliability standards (AEC-Q100) in mind is essential to eliminate field failures.

Disclaimer

The market data and statistics in this article reflect the information available at the time the cited sources were published. For the most current information, please refer to the official reports of the respective research organizations.
This page is a translation of the Japanese original. Some content may differ or reflect updates with a delay. For the most accurate and current information, please refer to the Japanese version as the official source.